Bangladesh Trial Cuts CVC Dyeing Steam Use 16.7% at 115°C

A carrier-assisted trial at N.A. Z Bangladesh cut CVC dyeing steam use 16.7% by dropping peak temperature to 115°C, saving 52 minutes per batch with rubbing fastness held at grade 4–5.

Fiber
Textile Innovation
Count
3 min read
Cut
Weight
687 words

Spec notes

  1. Steam consumption fell 16.7%, from 1.286 to 1.072 kg per kg fabric, at 115°C versus 130°C.
  2. Cycle time dropped from 222 to 170 minutes, a 52-minute saving and 23.4% calculated productivity gain.
  3. Trial ran on 42 kg of 80/20 CVC single jersey (180 GSM) at N.A. Z Bangladesh Ltd, commissioned by HI TECH.
  4. Rubbing fastness stayed at grades 3–4 to 4–5 across cotton, nylon, polyester, acrylic and wool components.
  5. Baseline and trial differed in fabric structure, GSM, batch size and shade; further matched trials are required.
An energy and steam saving alternative to conventional high-temperature polyester dyeing
Chip 01 · SW-9280An energy and steam saving alternative to conventional high-temperature polyester dyeing — wal_172619 / pixabay

A carrier-assisted dyeing trial at N.A. Z Bangladesh Ltd. has cut specific steam consumption on 80/20 CVC single jersey by 16.7%, lowering peak dyeing temperature from 130°C to 115°C. Steam use fell from 1.286 to 1.072 kg per kg of fabric. Total cycle time dropped from 222 to 170 minutes — a 52-minute saving per batch and a calculated productivity gain of 23.4%.

The industrial trial, commissioned by HI TECH and coordinated by Textile Today, was run on 180-GSM single jersey at a 42 kg batch weight. Khaled Faisal, GM of NAZ Bangladesh Ltd, supervised factory operations. Md. Mesbah Uddin, Technical Sales Manager at Transfar Chemicals, provided technical supervision. Sadia Afrin Mou, Anik Naha and Mita Akhter led the innovation team.

How does the chemistry work?

Polyester's hydrophobic, highly crystalline structure resists dye diffusion. Conventional disperse dyeing forces uptake at 130–140°C. Carriers swell the fiber and loosen its molecular structure, increasing free volume between polymer chains so dye molecules penetrate without full thermal energy. Dispersing agents keep dye particles suspended; levelling agents promote uniform distribution; mildly acidic pH supports exhaustion.

The trial formulation combined a carrier (TF-258WH), a dispersing agent, a levelling agent, an auxiliary stabilizer and acetic acid. TF-258WH's full chemistry remains undisclosed under industrial confidentiality agreements — a constraint on replication elsewhere.

What did the numbers show?

Researchers calculated heat demand as Q = M·S·Δθ, at a 1:6 liquor ratio, using water's 4.2 kJ/kg·°C specific heat. Steam enthalpy at 6 bar was set at 2,755.5 kJ/kg, with 36% total losses (distribution 6%, heat exchanger 10%, condensate 20%), giving effective enthalpy of 1,763.52 kJ/kg.

  • Baseline: 1,093.19 kg batch of CVC F-Terry (350 GSM), 6,559.14 kg water, 90°C rise, 2,479,354.92 kJ heat, 1,405.91 kg steam — 1.286 kg/kg fabric, 2,267.9 kJ/kg energy.
  • Trial: 42 kg batch, 252 kg water, 75°C rise, 79,380 kJ heat, 45.01 kg steam — 1.072 kg/kg fabric, 1,890.0 kJ/kg energy.
  • Savings per kg: 16.7% on both steam and energy; peak temperature 15°C lower.

The baseline heated at 1.5°C/min from 70°C to 130°C; the trial heated directly to 115°C. Both processes held peak temperature for 40 minutes.

Did quality hold?

Yes. The trial produced a level, uniform shade with no visible patchiness. Rubbing fastness grades on the 1–5 scale matched the baseline across fiber components.

  • Cotton: dry 4–5, wet 3–4 in both processes.
  • Nylon: dry 4–5, wet 2–3 in both.
  • Polyester: dry 4–5, wet 3–4 in both.
  • Acrylic: 4–5 color fastness, dry 4–5 in both.
  • Wool (trial only): 4–5, wet 4–5; baseline wool data unavailable.

What are the caveats for sourcing teams?

The comparison carries structural limitations. The baseline ran on 350-GSM F-Terry at 1,093.19 kg; the trial ran on 180-GSM single jersey at 42 kg. Fabric structure, GSM, batch size and shade all differed, which may affect dyeing kinetics. Factory management restricted testing to variables permitted in a live production setting, blocking broader pilot-scale work. Validation for deep shades and alternative blends remains outstanding.

What are the operational implications?

The study projects lower fuel and energy costs, reduced CO₂ emissions per kg of fabric, better machine utilization and more batches per shift. Lower chemical consumption and shorter process time also reduce effluent load to the ETP, cutting downstream wastewater treatment costs. The authors map the gains to SDG 7, 9 and 12.

The context matters for cost baselines. Conventional PC and CVC batches in Bangladesh can run up to 18 hours, and most large dyeing units still rely on the high-temperature route, sustaining high fuel bills and emissions.

Matched industrial trials across additional shades, blends and batch sizes are needed before the 16.7% steam saving and 23.4% productivity gain can be treated as reproducible at scale.

via textiletoday.com.bd (Source)

Filed under

Share this article:

More from Marcus Bennett

Marcus Bennett

Show full bio

Senior reporter covering money, funding and market shifts around fashion industry as a trade and business at The Fabric Brief.

308 articles

Also on the board

« Previous article